C, S determination in ore samples

閱讀:2659      發(fā)布時(shí)間:2015-05-15
分享:
  Suitable analyzers
n CS-800
n CS-2000 (induction furnace)
Used accessories
n Ceramic crucibles (90150)
n Tungsten (90220)
n Iron accelerator (90260)
n Suitable calibration material (NIST or other)
Settings
n Comparator level: 20 mV
n Minimum time: 40 sec
n Maximum time: 3:00 min
n Integration delay: 6 sec
n Post-waiting: 15 sec
n Pre-purging: 10 sec
n Base line deviation: 10 mV
Base line time: 15 sec
n T1 - Pre-purging: 5 sec
n T2 - Chamber only: 5 sec
n T3 - Chamber and lance: 3 sec
n T4 - Generator: 45 sec

Sample preparation
For best results grind the sample down to a particle size of approx. 200 µm.
Dry the sample to constant mass at 105°C (at least 1 hour).
Pre-heating the crucibles (1 h; 1000°C) could improve the precision.
Procedure
n Prepare ELTRA analyzer (e.g. exchange anhydrone, sodium hydroxide,
copper oxide when necessary); clean the combustions tube
n Run three warm up samples (e.g. steel samples (92400-3050) with a
minimum weight of 500 mg; add 1.5 g tungsten)
n Calibrate the analyzer with suitable calibration material (NIST or other)
(1) Weigh in 150 mg of sample in the ceramic crucibles (90150)
(2) Add 0.7 (±0.1) g of iron accelerator (90260) and 2.0 (±0.1) g of
tungsten (90220)
(3) Place the crucible on the pedestal and start analysis
Repeat Step (1) – (3) at least three times;
Mark the results and use the calibration function in the software.


提供商

弗爾德(上海)儀器設(shè)備有限公司

下載次數(shù)

232次

資料大小

347.4KB

資料類型

PDF 文件

資料圖片

--

瀏覽次數(shù)

2659次

會(huì)員登錄

請(qǐng)輸入賬號(hào)

請(qǐng)輸入密碼

=

請(qǐng)輸驗(yàn)證碼

收藏該商鋪

標(biāo)簽:
保存成功

(空格分隔,最多3個(gè),單個(gè)標(biāo)簽最多10個(gè)字符)

常用:

提示

您的留言已提交成功!我們將在第一時(shí)間回復(fù)您~
在線留言