  Suitable analyzers
n CS-800
n CS-2000 (induction furnace)
Used accessories
n Ceramic crucibles (90150)
n Tungsten (90220)
n Suitable calibration material (NIST or other)
Settings
n Comparator level: 10 mV
(low C, S Channel only)
n Minimum time: 45 sec
n Maximum time: 3:00 min
n Integration delay: 6 sec
n Post-waiting: 10 sec
n Pre-purging: 15 sec
n Base line deviation: 5 mV
Base line time: 30 sec
n T1 - Pre-purging: 5 sec
n T2 - Chamber only: 5 sec
n T3 - Chamber and lance: 1 sec
n T4 - Generator: 40 sec

Sample preparation
Make sure that the surface of the pure iron is free from contaminations;
otherwise clean the sample with acetone p.a. and let dry at atmosphere.
Pre-heat the crucibles at least 1 h at 1000°C ; let the crucibles cool down
in an exsiccator.
Procedure
n Prepare ELTRA analyzer (e.g. exchange anhydrone, sodium hydoxide,
copper oxide when necessary); clean the combustion tube, brush, heating
shield, dust trap
n Run three warm up samples (e.g. steel samples (92400-3050) with a
minimum weight of 500 mg; add 1.5 g tungsten)
n Calibrate the analyzer with suitable calibration material (NIST or other)
(1) Weigh in approx. 500 mg of sample in the ceramic crucibles (90150)
(2) Add 1.7 (±0.1 g) of tungsten (90220)
(3) Place the crucible on the pedestal and start analysis
Repeat step (1) - (3) at least three times;
Mark the results and use the calibration function in the software.


提供商

弗爾德(上海)儀器設(shè)備有限公司

下載次數(shù)

172次

資料大小

345.2KB

資料類型

PDF 文件

資料圖片

--

瀏覽次數(shù)

2690次

會員登錄

請輸入賬號

請輸入密碼

=

請輸驗證碼

收藏該商鋪

標(biāo)簽:
保存成功

(空格分隔,最多3個,單個標(biāo)簽最多10個字符)

常用:

提示

您的留言已提交成功!我們將在第一時間回復(fù)您~
在線留言